Exothermic Welding for Grounding Joints: How It Works, Where to Use It and What to Specify

Short answer: exothermic welding (also called thermite or aluminothermic welding, and widely known by the trade name cadweld) joins two copper or steel conductors by reducing copper oxide with aluminium inside a graphite mould and pouring the resulting molten copper into the joint cavity. The result is a molecular bond with the full current-carrying capacity of the conductor, no mechanical clamp to loosen, and no external power required on site. It is the reference method for buried ground-grid joints, down-conductor splices and steel-to-copper transitions — and it is the joint type most often written into lightning protection and substation earthing specifications.

Specify it when: the joint is buried or otherwise inaccessible, the design life exceeds 20 years, or the joint must survive a lightning impulse current without a resistance step. Use a bolted or compression connector instead where the joint must be removable for testing or where hot work is prohibited.

What actually happens inside the mould

Conclusion first: the reaction is self-sustaining once ignited and produces roughly 2500 °C of molten copper, which flows into the mould cavity, fuses the conductor ends and solidifies into a single piece of copper. There is no filler metal and no flux — the joint is not a soldered connection and behaves metallurgically like a continuous conductor.

  • The charge: a measured copper oxide + aluminium powder mix in a welded sealed cartridge, sized to the conductor cross-section. Cartridge size is the single most common ordering error — under-sized cartridges produce a cold, porous joint.
  • The mould: a two-piece graphite block machined to the exact joint geometry. Graphite survives the pour but is brittle; it is a consumable with a finite life, typically 50–100 pours depending on the profile and how carefully it is cleaned.
  • The sequence: clean and dry the conductors, seat them in the mould, clamp the mould, insert the cartridge and starting disc, close the lid, ignite, wait, then open and remove slag. Total cycle time per joint is a few minutes plus mould cleaning.

Which joints qualify

Joint typeTypical useNotes
Cable to cable (tee, splice, cross, parallel)Ground grid conductors, ring earth electrodesThe highest-volume application; mould profiles are standardised by conductor size
Cable to ground rodVertical earth electrode head, copper-bonded or galvanized rodRequires a rod-size-specific mould; check rod diameter before ordering
Cable to steel structureDown conductor to steel column, rebar, tower legUses a steel-surface mould half; surface must be ground bright and dry
Copper to galvanized steel transitionMixed-metal earth systemsRequires a dedicated transition cartridge to limit brittle intermetallic formation
Cable to busbar / plateEquipotential bonding bar, transformer neutralPlate thickness must match the mould cavity

For material selection upstream of the joint — copper-bonded versus galvanized steel conductors and rods — see our grounding conductor selection guide.

Defects that fail inspection, and their causes

Conclusion first: almost every failed exothermic joint traces back to one of four causes — wet or dirty conductors, a damp mould or cartridge, the wrong cartridge size, or a mould that was not clamped shut. The joint is unforgiving because the pour happens once and cannot be re-run on the same conductors without cutting them back.

  • Porous or spongy joint: moisture or contamination on the conductor, or a damp charge. Store cartridges dry and preheat the mould in humid conditions.
  • Incomplete fill / cold joint: cartridge too small for the cross-section, or heat lost to a cold, oversized steel member. Preheat heavy steel and step up one cartridge size.
  • Leakage fins: mould faces not closed tight, or a worn mould with a damaged sealing surface. Replace the mould rather than over-clamping a damaged one.
  • Conductor not fully seated: the cable was not pushed to the mould stop, so the weld metal bridged but did not fuse the full cross-section. Seat positively before igniting.

Acceptance is normally visual plus a hammer tap for buried work, with resistance measurement across the joint on critical circuits. Any joint showing less than full cross-section fusion should be cut out and remade — it cannot be repaired in place.

Source note: the reaction temperature and mould service-life figures above are typical industry working values for copper-oxide/aluminium exothermic systems. They are not measured values for any single product — confirm them against the cartridge and mould manufacturer's data sheet for the specific system being installed, and against the applicable earthing standard for the project.

Exothermic versus bolted versus compression

CriterionExothermic weldBolted connectorCompression (crimp)
Connection natureMolecular / metallurgical bondMechanical pressureMechanical pressure
Loosening over timeNone — no interface to loosenYes — needs periodic re-torqueLow, but depends on die and installer
Current capacityEqual to conductorLimited by contact areaLimited by contact area
Corrosion in buried serviceNo crevice to trap moistureCrevice corrosion riskCrevice corrosion risk
Survives lightning impulseYes, no resistance stepCan degrade at the interfaceGenerally yes if correctly crimped
Removable / testableNo — destructive to openYesNo
On-site power or toolingNone (just ignition source)Torque wrenchHydraulic or manual crimper
Hot-work permitUsually requiredNot requiredNot required
Skill sensitivityModerate — single irreversible pourLowModerate — die and crimp count

How to specify it in a procurement document

Conclusion first: specify the joint geometry, the conductor sizes and standards, the cartridge sizing rule and the acceptance criterion — not just "exothermic welding". Vague specs are where under-sized cartridges and mixed-metal failures enter a project.

  • Name the joint geometry and both conductor sizes (e.g. 120 mm² bare copper tee to 70 mm² bare copper), plus rod diameter or plate thickness where applicable.
  • State the cartridge sizing rule: cartridge selected by the manufacturer's table for the stated cross-section, with no field substitution.
  • Require matched moulds and cartridges from one system; mismatched graphite wear is a common cause of leakage fins.
  • Set the acceptance criterion: full cross-section fusion, no slag inclusion, no leakage beyond a stated fin dimension, and joint resistance not exceeding the equivalent conductor length.
  • Require trained installers and a pre-construction sample joint for destructive verification on large projects.

Liaocheng Feiyan New Material Technology Co., Ltd. supplies grounding and lightning-protection materials including copper-bonded and zinc-bonded steel, grounding rods and exothermic welding consumables, and supports joint specification and installer training on substation, telecom and photovoltaic projects. For designing the electrode system that these joints sit in, see how to reduce grounding resistance.

Frequently asked questions

Is an exothermic weld stronger than the conductor itself?

The joint is a molecular bond with the full current-carrying capacity of the conductor, so electrically and mechanically it performs as a continuous conductor rather than as a connection point. It has no contact interface that can loosen or corrode.

Can exothermic welding join copper to galvanized steel?

Yes, but it requires a dedicated copper-to-galvanized-steel transition cartridge and a steel-surface mould half. Using a standard copper cartridge on galvanized steel produces a brittle joint that can crack.

Do exothermic welds need maintenance?

No. Because there is no mechanical interface and no crevice, buried exothermic joints do not require periodic re-torquing or corrosion inspection, which is why they are specified for inaccessible joints.

What causes a porous or spongy exothermic weld?

Moisture or contamination on the conductors, or a damp cartridge or mould. Store cartridges dry, clean and brighten the conductor ends, and preheat the mould in humid conditions.

Is a hot-work permit required for exothermic welding?

In most jurisdictions yes, because the reaction produces an open flame and sparks. Where hot work is prohibited on site, a compression connector is the usual substitute, at the cost of a mechanical interface.

How many pours does a graphite mould last?

Typically 50 to 100 pours depending on the profile, the conductor size and how carefully the mould is cleaned between joints. A worn sealing surface causes leakage fins and should be replaced rather than over-clamped.

Business inquiries:
Precious Metal Recycling · Grounding Materials · Products · Contact Us
Tel 19963594228 | Office 0635-2112001 | Email fykj425@gmail.com
← Back to News

Liaocheng Feiyan New Material Technology Co., Ltd.

Address: Room 8-1503, 15F, Building 9, Xingguang International Financial Center, Dongchang East Road, Dongcheng Sub-district, Liaocheng Economic and Technological Development Area, Shandong, China

Tel: 0635-2112001 / 19963594228 | Email: fykj425@gmail.com

Copyright © Liaocheng Feiyan New Material Technology Co., Ltd.. All Rights Reserved.